I-CRAL 205 iyi-iron-chromium-aluminium alloy (i-FeCrAl alloy) ebonakala ngokumelana okuphezulu, i-coefficient ephansi yokumelana kagesi, izinga lokushisa eliphezulu lokusebenza, ukumelana okuhle kokugqwala ngaphansi kwezinga lokushisa eliphezulu. Ifanele ukusetshenziswa emazingeni okushisa afinyelela ku-1300°C.
Ukusetshenziswa okujwayelekile kwe-CRAL 205 kusetshenziswa esithandweni sikagesi sezimboni, esitofini sokupheka sikagesi se-ceramic.
Ukwakheka okuvamile%
| C | P | S | Mn | Si | Cr | Ni | Al | Fe | Okunye |
| Ubuningi | |||||||||
| 0.04 | 0.02 | 0.015 | 0.50 | Umkhawulo ongu-0.4 | 20.0-21.0 | Umkhawulo ongu-0.10 | 4.8-6 | Ibhalansi. | / |
Izakhiwo Ezijwayelekile Zomzimba
| Ubuningi (g/cm3) | 7.10 |
| Ukumelana kukagesi ku-20℃ (ohmm2/m) | 1.39 |
| I-coefficient yokuqhuba amandla ku-20℃ (WmK) | 13 |
| Amandla Okudonsa (i-Mpa) | 637-784 |
| Ukwelulwa | Ubuncane be-16% |
| I-Harness (HB) | 200-260 |
| Isilinganiso Sokunciphisa Ukwehluka Kwesigaba | 65-75% |
| Imvamisa Yokugoba Ngokuphindaphindiwe | Ubuncane izikhathi ezi-5 |
| Isilinganiso sokunwetshwa kokushisa | |
| Izinga lokushisa | I-Coefficient Yokwanda Kokushisa x10-6/℃ |
| 20 ℃ - 1000℃ | 16 |
| Umthamo wokushisa othize | |
| Izinga lokushisa | 20℃ |
| I-J/gK | 0.49 |
| Indawo yokuncibilika (℃) | 1500 |
| Izinga lokushisa eliphezulu lokusebenza eliqhubekayo emoyeni (℃) | 1300 |
| Izakhiwo zikamazibuthe | amandla kazibuthe |
150 0000 2421